Comhdhéanamh
Tábla 1 .Raonta comhdhéanamh tipiciúil le haghaidh cruach dhosmálta 304-grád
| Grád | C | Mn | Si | P | S | Cr | Mo | Ni | N | |
|---|---|---|---|---|---|---|---|---|---|---|
| 304 | nóim. uas. |
- 0.08 |
- 2.0 |
- 0.75 |
- 0.045 |
- 0.030 |
18.0 20.0 |
- | 8.0 10.5 |
- 0.10 |
| 304L | nóim. uas. |
- 0.030 |
- 2.0 |
- 0.75 |
- 0.045 |
- 0.030 |
18.0 20.0 |
- | 8.0 12.0 |
- 0.10 |
| 304H | nóim. uas. |
0.04 0.10 |
- 2.0 |
- 0.75 |
-0.045 | - 0.030 |
18.0 20.0 |
- | 8.0 10.5 |
- |
Airíonna Meicniúla
Tábla 2 .Airíonna meicniúla tipiciúla déanta as cruach dhosmálta 304-grád
| Grád | Neart Teanntachta (MPa) min | Neart Toradh 0.2% Cruthúnas (MPa) min | Fadú (% i 50 mm) min | Cruas | |
|---|---|---|---|---|---|
| Rockwell B (HR B) max | Brinell (HB) max | ||||
| 304 | 515 | 205 | 40 | 92 | 201 |
| 304L | 485 | 170 | 40 | 92 | 201 |
| 304H | 515 | 205 | 40 | 92 | 201 |
Éilíonn 304H freisin méid gráin ASTM Uimh 7 nó níos garbh.
Airíonna Fisiceacha
Tábla 3 .Airíonna fisiceacha tipiciúla cruach dhosmálta 304-grád sa riocht annealed
| Grád | Dlús (kg/m3) | Modal Leaisteacha (GPa) | Meán Chomhéifeacht Leathnaithe Teirmeach (μm/m/ céim ) | Seoltacht Theirmeach (W/mK) | Teas Sonrach 0-100 céim (J/kg.K) | Friotaíocht Leictreach (nΩ.m) | |||
|---|---|---|---|---|---|---|---|---|---|
| 0-100 céim | 0-315 céim | 0-538 céim | ag 100 céim | ag 500 céim | |||||
| 304/L/H | 8000 | 193 | 17.2 | 17.8 | 18.4 | 16.2 | 21.5 | 500 | 720 |
Comparáid Sonraíocht Grád
Tábla 4 .Sonraíochtaí Neas Grád le haghaidh cruach dhosmálta 304-grád
| Grád | UNS Uimh | Sean Briotanach | Euronorm | SS Sualainnis | JIS na Seapáine | ||
|---|---|---|---|---|---|---|---|
| BS | En | Níl | Ainm | ||||
| 304 | S30400 | 304S31 | 58E | 1.4301 | X5CrNi18-10 | 2332 | SUS 304 |